All Properties - Our Standard Alloys

 Alloy

                319

356

535

713

 Temper

F

T6

F

T6

F

F

 Tensile Strength

27000

36000

24000

33000

40000

35000

 Yield Strength

18000

24000

18000

24000

21000

25000

 Elongation % in 2”

2

2

6

3.5

9

5

 Brinell Hardness

70

80

65

70

70

74

 Shear Strength

22000

29000

 

26000

28000

 

 Endurance Limit

10000

11000

 

8500

10000

 

 Fluidity*

2

1

3

4

 Pressure Tightness*

2

1

5

4

 Hot Strength*

2

1

3

5

 Corrosion Resistance*

3

2

1

2

 Machinability*

3

4

1

1

 Elevated Temp Strength*

3

3

3

5

 Anodizing Quality*

4

4

 

2

 Specific Gravity

2.79

2.68

2.62

2.81

 Weight – lbs. per cu. in.

.101

.097

.095

.100

 Avg Melting Point

1040

1085

1092

1140

 Electrical  Conductivity                       % of AICS

27

39

23

37

 Thermal  Conductivity                   CGS

.26

.36

.24

.29

Coefficient of     Thermal Expansion    (in/in/F*10-6)

60-212F

60-572F

11.9

11.9

13.1

13.4

12.7

12.9

14.8

14.6

1)Properties 30 days after casing.     2) Values in PSI units.      3) 500kg/10mm Ball.