Typical Mechanical Properties - All Alloys |
|||||||
Alloy and Temper |
Tensile
Strength |
Yield Strength |
Elongation % in
2" |
Brinell
Hardness |
Shear Strength |
Endurance Limit |
|
A206.0 |
T4 |
51000 |
36000 |
7 |
|
40000 |
|
208.0 |
F |
21000 |
14000 |
2.5 |
55 |
17000 |
11000 |
295.0 |
T4 |
32000 |
16000 |
9 |
60 |
26000 |
7000 |
295.0 |
T6 |
36000 |
24000 |
5.0 |
75 |
30000 |
7500 |
319.0 |
F |
27000 |
18000 |
2 |
70 |
22000 |
10000 |
319.0 |
T5 |
30000 |
26000 |
1.5 |
80 |
24000 |
11000 |
319.0 |
T6 |
36000 |
24000 |
2 |
80 |
29000 |
11000 |
355.0 |
F |
23000 |
12000 |
3 |
65 |
28000 |
9000 |
355.0 |
T6 |
35000 |
25000 |
3 |
80 |
28000 |
9000 |
C355.0 |
F |
27000 |
16000 |
2.5 |
65 |
|
|
C355.0 |
T6 |
38000 |
28000 |
5 |
90 |
28000 |
10000 |
356.0 |
F |
24000 |
18000 |
6 |
65 |
|
|
356.0 |
T6 |
33000 |
24000 |
3.5 |
70 |
26000 |
8500 |
A356.0 |
F |
23000 |
12000 |
6 |
55 |
|
|
A356.0 |
T6 |
37000 |
27000 |
5 |
80 |
|
|
361.0 |
T6 |
38000 |
26000 |
3 |
75 |
30000 |
|
443.0 |
F |
19000 |
8000 |
8 |
40 |
14000 |
8000 |
514.0 |
F |
25000 |
12000 |
9 |
50 |
20000 |
7000 |
520.0 |
T4 |
48000 |
26000 |
16 |
75 |
34000 |
8000 |
535.0 |
F |
40000 |
21000 |
13 |
70 |
28000 |
10000 |
712.0 |
T5 |
35000 |
25000 |
5 |
75 |
26000 |
8000 |
713.0 |
T5 |
35000 |
25000 |
5 |
75 |
26000 |
9000 |
771.0 |
T5 |
42000 |
35000 |
5 |
90 |
|
|
850.0 |
T5 |
20000 |
11000 |
6 |
45 |
14000 |
|
852.0 |
T5 |
27000 |
22000 |
2 |
65 |
18000 |
10000 |
1) Properties 30 days after casing. 2) Values in PSI units. 3) 500kg/10mm Ball.